The influence of synthesis temperature on the structural and electrical properties of metal-dielectric-semiconductor structures based on hafnium oxide films
M.S. Afanasiev, D.A. Belorusov, E.I. Goldman, D.A. Kiselev, A.A. Sivov, G.V. Chucheva
Fryazino branch of the Kotelnikov Institute of Radioengineering and Electronics of RAS
DOI: 10.26456/pcascnn/2026.18.530
Original article
Abstract: In this work, hafnium oxide films were obtained on silicon substrates using magnetron sputtering at temperatures of 25, 300, 500, and 700°C. The results of scanning probe microscopy studies of the quality of HfO2 films and the electrophysical properties of metal-dielectric-semiconductor structures (Ni-HfO2-Si) are presented. It is shown that an increase in the synthesis temperature enlarges the crystallites (from 53 to 100 nm) and reduces the roughness. At a synthesis temperature of 500°C, an improvement in the ferroelectric parameters is observed: the built-in voltage decreases from +1,38 to +0,33 V, and the loop squareness coefficient increases from 0,34 to 0,63. The largest loop width on the capacitance-voltage characteristic (~4 V) and the best frequency stability of capacitance and dielectric losses are achieved at a synthesis temperature of 300°C. A further increase in temperature to 500-700°C increases the maximum capacitance, but narrows the hysteresis loop, reduces frequency stability, and shifts the minimum of dielectric losses to the high-frequency region. It is determined that the saturation of the field curves of high-frequency capacitances is not associated with the inversion of Si at the Si/HfO2 contact during semiconductor depletion and is not associated with deep enrichment of the silicon surface, but is due to the pinning of the Fermi level on the branches of the U-shaped density of states of electron traps in the buffer layer between the substrate and the insulating layer. It is established that the choice of the synthesis temperature allows for targeted control of the film properties: 500°C is optimal for enhancing the ferroelectric response, while 300°C is optimal for obtaining frequency-stable structures. The results are useful for the development of non-volatile memory and high-frequency devices based on HfO2.
Keywords: ferroelectric films, hafnium oxide (HfO2), structures metal-dielectric-semiconductor, electrophysical properties, polarization
- Mikhail S. Afanasiev – Dr. Sc., Associate Professor, Leading Researcher, Fryazino branch of the Kotelnikov Institute of Radioengineering and Electronics of RAS, ORCID: 0000-0001-5475-8616
- Dmitriy A. Belorusov – Researcher, Fryazino branch of the Kotelnikov Institute of Radioengineering and Electronics of RAS
- Evgeniy I. Goldman – Ph. D., Leading Researcher, Fryazino branch of the Kotelnikov Institute of Radioengineering and Electronics of RAS
- Dmitriy A. Kiselev – Ph. D., Senior Researcher, Fryazino branch of the Kotelnikov Institute of Radioengineering and Electronics of RAS, ORCID: 0000-0003-1047-3007
- Alexey A. Sivov – Researcher, Fryazino branch of the Kotelnikov Institute of Radioengineering and Electronics of RAS
- Galina V. Chucheva – Dr. Sc., Chief Researcher, Fryazino branch of the Kotelnikov Institute of Radioengineering and Electronics of RAS, ORCID: 0000-0002-9956-1857
For citation:
Afanasiev M.S., Belorusov D.A., Goldman E.I., Kiselev D.A., Sivov A.A., Chucheva G.V. Vliyanie temperatury sinteza na strukturnye i elektricheskie svojstva struktur metall-dielektrik-poluprovodnik na osnove plenok oksida gafniya [The influence of synthesis temperature on the structural and electrical properties of metal-dielectric-semiconductor structures based on hafnium oxide films], Fiziko-khimicheskie aspekty izucheniya klasterov, nanostruktur i nanomaterialov [Physical and chemical aspects of the study of clusters, nanostructures and nanomaterials], 2026, issue 18, pp. 530-540. DOI: 10.26456/pcascnn/2026.18.530. ⎘
Full article (in Russian): download PDF file
References:
1. Vorotilov К.А., Muhortov V.М., Sigov А.S. Integrirovannye segnetoelektricheskie ustroystva [Integrated ferroetoelectric devices]. Moscow, Energoatomizdat Publ., 2011. – 175 p. (In Russian).
2. Park J.Y., Yang K., Lee D.H. et al. A perspective on semiconductor devices based on fluorite-structured ferroelectrics from the materials–device integration perspective, Journal of Applied Physics, 2020, vol. 128, issue 24, art. no. 240904, 24 p. DOI: 10.1063/5.0035542.
3. Böscke T.S., Müller J., Bräuhaus D. et al. Ferroelectricity in hafnium oxide thin films, Applied Physics Letters, 2011, vol. 99, issue 10, art. no. 102903, 4 p. DOI: 10.1063/1.3634052.
4. Müller J., Böscke T.S., Bräuhaus D. et al. Ferroelectric Zr0.5Hf0.5O2 thin films for nonvolatile memory applications, Applied Physics Letters, 2011, vol. 99, issue 11, art. no. 112901, 4 p. DOI: 10.1063/1.3636417.
5. Paul A., Kumar G., Das A. et al. Hafnium oxide-based ferroelectric field effect transistors: From materials and reliability to applications in storage-class memory and in-memory computing, Journal of Applied Physics, 2025, vol. 138, issue 1, art. № 010701, 19 p. DOI: 10.1063/5.0278057.
6. Khaskheli M.A., Wu P., Li X. et al. Effects of substrate temperature on dielectric and structural properties of Ti and Er co-doped HfO2 thin films, Vacuum, 2012, vol. 86, issue 12, pp. 1920-1923. DOI: 10.1016/j.vacuum.2012.03.028.
7. Das K.C., Ghosh S.P., Tripathy N. et al. Evolution of microstructural and electrical properties of sputtered HfO2 ceramic thin films with RF power and substrate temperature, Ceramics International, 2016, vol. 42, issue 1, pp. 138-145. DOI: 10.1016/j.ceramint.2015.08.038.
8. Nath M., Roy A. Interface and electrical properties of ultra-thin HfO2 film grown by radio frequency sputtering, B: Condensed Matter, 2016, vol. 482, pp. 43-50. DOI: 10.1016/j.physb.2015.12.007.
9. Gol'dman E.I., Zhdan A.G., Chucheva G.V. Determination of the coefficients of ion transfer in insulating layers on the surface of semiconductors using dynamic current-voltage depolarization characteristics, Instruments and Experimental Techniques, 1997, vol. 40, issue 2, pp. 841-846.
10. Gwyddion – Free SPM (AFM, SNOM/NSOM, STM, MFM, …) data analysis software. Available at: http://gwyddion.net (accessed 15.07.2026).
11. Goldman E.I., Chucheva G.V., Belorusov D.A. On the form of high-frequency voltage-capacitance characteristics of metal-insulator-semiconductor structures with a ferroelectric insulating layer BaxSr1-хTiO3, Ceramics International, 2021, vol. 47, issue 15, pp. 21248-21252. DOI: 10.1016/j.ceramint.2021.04.129.
12. Goldman E.I., Chucheva G.V., Belorusov D.A. The role of а buffer layer at the contact with silicon in structures with an insulating gap made of a material replacing SiO2, Ceramics International, 2024, vol. 50, issue 6, pp. 9678-9681. DOI: 10.1016/j.ceramint.2023.12.286.
13. Sze S.M., Ng K.K. Physics of semiconductor devices, 3rd edition. Hoboken, John Willey & Sons, 2007, 815 p.