Physical and chemical aspects of the study of clusters, nanostructures and nanomaterials. Founded at 2009


Features of zirconium carbonitride formation under multistage reduction-carburization-nitridation of ZrO2

S.N. Yudin1, A.V. Kasimtsev2, S.S. Volodko1, D.O. Moskovskikh1

1 National University of Science and Technology MISIS
2 METSINTEZ LLC

DOI: 10.26456/pcascnn/2026.18.197

Original article

Abstract: The nitridation of products obtained by calcium hydride reduction–carburization of ZrO2 at 1200°C was studied with the aim of synthesizing zirconium carbonitride ZrCxN1-x. The effect of nitriding duration (ranging from 1 to 12 hours) in a stationary nitrogen atmosphere at a pressure of 1,1 atm on the elemental and phase composition of the powders was investigated. Increasing the holding time did not result in a systematic increase in nitrogen content: the carbon and nitrogen concentrations were of approximately 40 and 6–8 at.%, respectively (C/N ≈ 5,5). X-ray diffraction analysis showed that, regardless of the nitridation time, a B1-type phase with the lattice parameter of 0,4691 nm was formed, corresponding to nearly pure ZrC. Energy-dispersive X-ray spectroscopy analysis indicated a local enrichment in nitrogen, predominantly at the protruding regions of the carbide particles. It was shown that at 1200°C nitridation of ZrC proceeds only to a limited extent and does not result in the formation of a homogeneous ZrCxN1-x carbonitride phase. It is suggested that the incompleteness of gas-phase (N2) nitriding processes is due to the formation of solid cyanamide (CaCN2), which physically blocks nitrogen access to the ZrC surface. It is shown that the nitriding products inherit the particle morphology of the synthesized ZrC carbide and are characterized by a nanodisperse structure.

Keywords: zirconium carbonitride, zirconium carbide, calcium hydride synthesis, reduction-carburization, nitridation, ZrO2

  • Sergey N. Yudin – Ph. D, Senior Researcher, «Engineering Ceramic Nanomaterials» Research Center, National University of Science and Technology MISIS, ORCID: 0000-0002-0531-002X
  • Anatoliy V. Kasimtsev – Dr. Sc., Professor, Director, METSINTEZ LLC
  • Sergey S. Volodko – Ph. D., Leading Expert of the Research Project, «Engineering Ceramic Nanomaterials» Research Center, National University of Science and Technology MISIS, ORCID: 0000-0001-6309-8218
  • Dmitriy O. Moskovskikh – Dr. Sc., Docent, Director, «Engineering Ceramic Nanomaterials» Research Center, National University of Science and Technology MISIS, ORCID: 0000-0001-5168-4885

For citation:

Yudin S.N., Kasimtsev A.V., Volodko S.S., Moskovskikh D.O. Osobennosti obrazovaniya karbonitrida tsirkoniya v usloviyakh mnogostadijnogo protsessa vosstanovleniya-karbidizatsii-azotirovaniya oksida ZrO2 [Features of zirconium carbonitride formation under multistage reduction-carburization-nitridation of ZrO2], Fiziko-khimicheskie aspekty izucheniya klasterov, nanostruktur i nanomaterialov [Physical and chemical aspects of the study of clusters, nanostructures and nanomaterials], 2026, issue 18, pp. 197-213. DOI: 10.26456/pcascnn/2026.18.197. ⎘

Full article (in Russian): download PDF file

References:

1. Andrievskii R.A. The synthesis and properties of nanocrystalline refractory compounds, Russian Chemical Reviews, 1994, vol. 63, no. 5, pp. 411-427. DOI: 10.1070/rc1994v063n05abeh000094.
2. Yang Q., Lengauer W., Koch T. et al. Hardness and elastic properties of Ti(CxN1-x), Zr(CxN1-x) and Hf(CxN1-x), Journal of Alloys and Compounds, 2000, vol. 309, issue 1-2, pp. L5-L9. DOI: 10.1016/S0925-8388(00)01057-4.
3. Lengauer W., Binder S., Aigner K. et al. Solid state properties of group IVb carbonitrides, Journal of Alloys and Compounds, 1995, vol. 217, issue 1, pp. 137-147. DOI: 10.1016/0925-8388(94)01315-9.
4. Zhang S. Material development of titanium carbonitride-based cermets for machining application, Key engineering materials, 1997, vol. 138-140, pp. 521-544. DOI: 10.4028/www.scientific.net/kem.138-140.521.
5. Bellosi A., Calzavarini R., Faga M.G. et al. Characterisation and application of titanium carbonitride-based cutting tools, Journal of Materials Processing Technology, 2003, vol. 143-144, pp. 527-532. DOI: 10.1016/S0924-0136(03)00339-X.
6. Guu Y.Y., Lin J.F. Analysis of wear behaviour of titanium carbonitride coatings, Wear, 1997, vol. 210, issue 1-2, pp. 245-254. DOI: 10.1016/S0043-1648(97)00056-2.
7. Guu Y.Y., Lin J.F., Ai C.-F. The tribological characteristics of titanium nitride, titanium carbonitride and titanium carbide coatings, Thin Solid Films, 1997, vol. 302, issue 1-2, pp. 193-200. DOI: 10.1016/S0040-6090(96)09546-6.
8. Kuzmenko E., Matrenin S., Nassyrbayev A. Oxidation behavior and physico-mechanical properties of spark plasma sintered ZrCN-ZrO2 ceramics, Ceramics International, 2025, vol. 51, issue 28, part A, pp. 56792-56803. DOI: 10.1016/j.ceramint.2025.09.393.
9. Kim J., Suh Y.J. Temperature- and pressure-dependent elastic properties, thermal expansion ratios, and minimum thermal conductivities of ZrC, ZrN, and Zr(C0.5N0.5), Ceramics International, 2017, vol. 43, issue 15, pp. 12968-12974. DOI: 10.1016/j.ceramint.2017.06.195.
10. Harrison R.W., Lee W.E. Processing and properties of ZrC, ZrN and ZrCN ceramics: a review, Advances in Applied Ceramics, 2016, vol. 115, issue 5, pp. 294-307. DOI: 10.1179/1743676115Y.0000000061.
11. Mazzoni A.D., Aglietti E.F. Formation of ZrX (O-N-C) phase by the carbonitriding of zircon at high temperatures, Materials Chemistry and Physics, 2000, vol. 65, issue 2, pp. 166-172. DOI: 10.1016/S0254-0584(00)00233-9.
12. Harrison R., Rapaud O., Pradeilles N. et al. On the fabrication of ZrCxNy from ZrO2 via two-step carbothermic reduction-nitridation, Journal of the European Ceramic Society, 2015, vol. 35, issue 5, pp. 1413-1421. DOI: 10.1016/j.jeurceramsoc.2014.11.005.
13. Harrison R., Ridd O., Jayaseelan D.D., Lee W.E. Thermophysical characterisation of ZrCxNy ceramics fabricated via carbothermic reduction-nitridation, Journal of Nuclear Materials, 2014, vol. 454, issue 1-3, pp. 46-53. DOI: 10.1016/j.jnucmat.2014.07.030.
14. Mazzoni A.D., Conconi M.S. Study of carbonitriding reactions of zirconia. Synthesis of Zr(C,N,O) phases and β-type zirconium oxynitrides, Ceramics international, 2004, vol. 30, issue 1, pp. 23-29. DOI: 10.1016/S0272-8842(03)00057-9.
15. Portnoy K.I., Levinsky Yu.V. Vzaimodejstvie v sistemakh tugoplavkie metally-uglerod-azot [Interaction in refractory metal-carbon-nitrogen systems], Issledovanie Splavov Tsvetnykh Metallov [Research of Non-Ferrous Metal Alloys]. Moscow, USSR Academy of Sciences Publishing House, 1963, vol. 4, pp. 279-385. (In Russian).
16. Cruz Fernandes J., Amaral P.M., Guerra Rosa L. et al. X-ray diffraction characterization of carbide and carbonitride of Ti and Zr prepared through reaction between metal powders and carbon powders (graphitic or amorphous) in a solar furnace, International Journal of Refractory Metals and Hard Materials, 1999, vol. 17, issue 6, pp. 437-443. DOI: 10.1016/S0263-4368(99)00036-0.
17. Johnson W.C., Stubbs M.F., Sidwell A.E., Pechukas A. The rate of formation and the dissociation of calcium hydride, Journal of the American Chemical Society, 1939, vol. 61, issue 2, pp. 318-329. DOI: 10.1021/ja01871a026.
18. Tripp H.P., King B.W. Thermodynamic data on oxides at elevated temperatures, Journal of the American Ceramic Society, 1955, vol. 38, issue 12, pp. 432-437. DOI: 10.1111/j.1151-2916.1955.tb14569.x.
19. Kubaschewski O., Dench W.A. The dissociation pressures in the zirconium-oxygen system at 1000 °C, Journal of the Institute of Metals, 1956, vol. 84, pp. 440-444.
20. Kasimtsev A.V., Zhigunov V.V. The mechanism and kinetics of producing single-crystal powders of titanium carbide via a hydride-calcium method, Russian Journal of Non-Ferrous Metals, 2008, vol. 49, issue 6, pp. 471-477. DOI: 10.3103/S1067821208060072.
21. Kasimtsev A.V., Tabachkova N.Y., Voldman G.M., Yudin S.N. Metal-thermal synthesis and properties of ultra-and nanopowders of titanium carbide, Tsvetnye Metally, 2014, no. 7, pp. 54-55.
22. Kasimtsev A.V., Yudin S.N., Levinsky Yu.V. Calciothermic powders of rare metals and intermetallic compounds, Non-Ferrous Metals, 2020, no. 2, pp. 31-50. DOI: 10.17580/nfm.2020.02.05.
23. Shelekhov E.V., Sviridova T.A. Programs for X-ray analysis of polycrystals, Metal Science and Heat Treatment, 2000, vol. 42, issue 8, pp. 309-313. DOI: 10.1007/BF02471306.
24. Grigorovich K.V., Alpatov A.V., Rumyantsev B.A. et al. Concentration and state of light elements in titanium carbide nanopowders, Inorganic Materials, 2015, vol. 51, issue 5, pp. 451-459. DOI: 10.1134/S0020168515050039.
25. Jacob K.T., Raj S., Rannesh L. Vegard’s law: a fundamental relation or an approximation?, International Journal of Materials Research, 2007, vol. 98, issue 9, pp. 776-788. DOI: 10.3139/146.101545.
26. Volodko S., Moskovskikh D., Yudin S. et al. Synthesis of nano- and ultra-fine refractory carbide powders by low-temperature calcium-carbothermic process and their grain growth during sintering, Ceramics international, 2024, vol. 50, issue 12, pp. 22141-22148. DOI: 10.1016/j.ceramint.2024.03.327.
27. Wu K.-H., Wang Y., Chou K.-C., Zhang G.-H. Low-temperature synthesis of single-phase refractory metal compound carbides, International Journal of Refractory Metals and Hard Materials, 2021, vol. 98, article no. 105567, 9 p. DOI: 10.1016/j.ijrmhm.2021.105567.
28. Abdelkader A.M., El-Kashif E. Calciothermic reduction of zirconium oxide in molten CaCl2, ISIJ International, 2007, vol. 47, issue 1, pp. 25-31. DOI: 10.2355/isijinternational.47.25.
29. Yamanaka M., Fujita Y., McLean A., Iwase M. A thermodynamic study of CaCN2, High Temperature Materials and Processes, 2000, vol. 19, issue 3-4, pp. 275-280. DOI: 10.1515/HTMP.2000.19.3-4.275.
30. Pickles C.A., Toguri J.M. Thermodynamic analysis of the Ca-C-N system, High Temperature Materials and Processes, 2004, vol. 23, issue 5-6, pp. 405-418. DOI: 10.1515/HTMP.2004.23.5-6.405.
31. Pang L.-L., Bi J.-Q., Bai Y.-J. et al. Rapid synthesis of graphitic carbon nitride powders by metathesis reaction between CaCN2 and C2Cl6, Materials Chemistry and Physics, 2008, vol. 112, issue 3, pp. 1124-1128. DOI: 10.1016/j.matchemphys.2008.07.053.
32. Meerson G.A., Olesov Y.G., Pryalochnikov V.I. The reduction of zirconium dioxide by calcium carbide and cyanamide, Soviet Atomic Energy, 1964, vol. 14, issue 6, pp. 586-592. DOI: 10.1007/BF01119974.
33. Yudin S.N., Kasimtsev A.V., Volodko S.S. et al. Low-temperature synthesis of ultra-high-temperature HfC and HfCN nanoparticles, Materialia, 2022, vol. 22, art. no. 101415, 13 p. DOI: 10.1016/j.mtla.2022.101415.

Content |